Reaktionsgleichung
O.O.O.O.O.O.[N+]([O-])([O-])=[O:8].[Co+2:11].[N+]([O-])([O-])=[O:13].O.O.O.O.O.O.O.O.O.[N+]([O-])([O-])=[O:26].[Al+3:29].[N+]([O-])([O-])=[O:31].[N+]([O-])([O-])=[O:35].C(=O)([O-])[O-].[NH4+].[NH4+]>O>[O-2:8].[O-2:13].[O-2:26].[O-2:31].[O-2:35].[Al+3:29].[Al+3:29].[Co+2:11].[Co+2:11]Komponenten
5
Edukt 3
Produkt 1
Reagenzien, Katalysatoren, Lösungsmittel 1
Versuchsvorschrift
In 300 ml of pure water were dissolved 29 g of cobalt nitrate hexahydrate and 75 g of aluminum nitrate nonahydrate. A solution of 38.4 g of ammonium carbonate dissolved in 100 ml of pure water was gradually added thereto with stirring to form a gel-form precipitate. The precipitate was washed with pure water three times, dried at 100° C. overnight and calcined at 600° C. in an air stream. The calcined material was then calcined at 800° C. in a muffle furnace for 3 hours to a cobalt aluminate catalyst having a blue color.
Aufarbeitung
- additionwas gradually added
- customto form a gel-form precipitate
- washThe precipitate was washed with pure water three times
- customdried at 100° C. overnight
- customcalcined at 600° C. in an air stream
Quellen und Nachweise
- ORD-Eintrag
- ord-d755ad4082d34d449f7b2c97f1c17329
- Quelldatensatz
- uspto-grants-1993_07
- Patentnummer
- US05227145
Verknüpfte Notizen
Wird geladen…