[O-2].[Zn+2:2].[C:3]1([P:9](=[O:12])([OH:11])[OH:10])[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1>C(O)C.O>[C:3]1([P:9](=[O:10])([O-:12])[O-:11])[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1.[Zn+2:2]A slurry in ethanol-water of zinc oxide was prepared by charging a 300 mL reaction flask equipped with a stirrer with 10.0 g (123 mmol) of zinc oxide (JIS grade 2, available from HakusuiTech Ltd.) and 90.0 g of 50% by mass ethanol-water. A solution of 1.9 g (12 mmol) of phenylphosphonic acid (Nissan Chemical Industries, Ltd.) dissolved in 11.0 g of 50% by mass ethanol-water was gradually added dropwise at room temperature (about 25° C.) to this slurry with stirring, thereby effecting a reaction for one hour. The slurry was then filtered and the wet cake was thoroughly rinsed with ethanol. The wet cake was subsequently dried at 120° C. for at least 12 hours, yielding a white powder of zinc phenylphosphonate-containing zinc oxide.