[C:1]([OH:10])(=[O:9])[CH2:2][CH2:3][CH2:4][CH2:5][C:6]([OH:8])=[O:7].[CH2:11]([C:13]([CH2:18][OH:19])([CH2:16][OH:17])[CH2:14][CH3:15])[OH:12].C1(C)C=CC=CC=1>O>[C:1]([OH:10])(=[O:9])[CH2:2][CH2:3][CH2:4][CH2:5][C:6]([OH:8])=[O:7].[CH2:11]([C:13]([CH2:18][OH:19])([CH2:16][OH:17])[CH2:14][CH3:15])[OH:12]Adipic acid (702 g, 4.8 mol), trimethylolpropane (537 g, 4 mol), 2.4 g of Fascat® and 200 g of toluene were heated to 125–130° C. under nitrogen and water formed was separated off using a water separator. After a reaction time of 11 hours, the toluene was distilled off under reduced pressure. The viscous, hyperbranched polyester was soluble in butyl acetate or THF but insoluble in water.