Reaction equation
[CH2:1]([O:5][C:6](=[O:9])[CH:7]=[CH2:8])[CH2:2][CH2:3][CH3:4].[CH2:10]=[CH:11][C:12]1[CH:17]=[CH:16][CH:15]=[CH:14][CH:13]=1.[K].S(OOS([O-])(=O)=O)([O-])(=O)=O.[K+].[K+]>O>[CH2:1]([O:5][C:6](=[O:9])[CH:7]=[CH2:8])[CH2:2][CH2:3][CH3:4].[CH2:10]=[CH:11][C:12]1[CH:17]=[CH:16][CH:15]=[CH:14][CH:13]=1Participants
Reactant 4
Product 1
Reagents, catalysts & solvents 1
Conditions
- Temperature
- 60 °C
Procedure
In a 200-liter reactor equipped with a stirrer, a cooling apparatus, a condenser and a monomer supplying tube, 5 parts by weight of butylacrylate, 15 parts by weight of styrene, 0.2 parts by weight of triallyl isocyanurate, 140 parts by weight of ion-exchanged water and 1.0 parts by weight of potassium rosinate are added and mixed. The temperature is raised to 60° C. with stirring. After 10 minutes from the time of reaching 60° C., 0.25 parts by weight of potassium persulfate dissolved in deionized water is added thereto to initiate polymerization. The temperature of the reactor is maintained at 70° C. for 60 minutes. The polymerization is carried out at 70° C. for an additional 30 minutes to give an inner core of butylacrylate-styrene copolymer.
Workup
- customIn a 200-liter reactor equipped with a stirrer
- additionmixed
- additionis added
- custompolymerization
- temperatureThe temperature of the reactor is maintained at 70° C. for 60 minutes
- waitThe polymerization is carried out at 70° C. for an additional 30 minutes
Sources & evidence
- ORD record
- ord-6308c29c53df4acabed5aeb9c47e1454
- Source dataset
- uspto-grants-2013_02
- Patent number
- US08367770B2
Linked notes
Loading…