CC(CCCC[N:13]=[C:14]=[O:15])C(N=C=O)(C)C.[CH3:16][CH2:17]C[CH2:19][CH:20]([C:23]([O-:25])=[O:24])[CH2:21]C.CCC[CH2:29][CH:30]([C:33]([O-:35])=[O:34])[CH2:31]C.[Sn+2]>>[C:23]([OH:25])(=[O:24])[C:20]([CH3:21])=[CH2:19].[C:33]([OH:35])(=[O:34])[C:30]([CH3:31])=[CH2:29].[NH2:13][C:14]([O:15][CH2:16][CH3:17])=[O:34]参加物
3
実験手順
To a mechanically-stirred mixture of 28.59 weight parts of trimethylhexamethylene diisocyanate and 0.04 weight part of stannous octoate in a reactor and purged with dry air, there is added 44.80 weight parts of polytetramethylene ether glycol, while maintaining the reaction temperature at 50° to 60° C. After the addition is complete, the mixture is heated to 70° to 80° C. and held for 3 hours. A 26.58 weight parts of hydroxyethyl methacrylate (HEMA) was added and the mixture was stirred at 70° to 80° C. until the percent NCO assay was below 0.01%.
後処理
- custompurged
- customwith dry air, there
- additionis added 44.80 weight parts of polytetramethylene ether glycol
- temperaturewhile maintaining the reaction temperature at 50° to 60° C
- additionAfter the addition
- temperaturethe mixture is heated to 70° to 80° C.
- additionA 26.58 weight parts of hydroxyethyl methacrylate (HEMA) was added
出典と根拠
- ORDレコード
- ord-da0fdd3ad703426f857a99254d42abae
- 出典データセット
- uspto-grants-1989_03
- 特許番号
- US04814423