反応手順
In a glass polymerization bottle were charged 80 g isooctyl acrylate (IOA), 18 g isobornyl acrylate (IBA), 2 g vinyldimethylazlactone (VDM), 100 g ethyl acetate, 0.5 g benzoyl peroxide and 0.04 g carbon tetrabromide. The bottle was purged with nitrogen, sealed and tumbled in a water bath maintained at 60° C. for 12 hours to produce a IOA/IBA/VDM terpolymer. The polymer was isolated by precipitation in isopropanol and dried under vacuum.
情報源と証拠
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| 特許番号 | US06448337B1 |
|---|
| 出典データセット | uspto-grants-2002_09 |
|---|
| ORD ID | ord-0f178365228a4680a63c0489ca01ac42 |
|---|
| 出典メモ | uspto-grants-2002_09 |
|---|