HRID1279668

反应详情

EQUATION

反应方程式

HRID 1279668 的结构方程式

AUXILIARIES

试剂、催化剂与溶剂

1

CONDITIONS

反应条件

温度
60 °C

PROCEDURE

实验过程

In a glass polymerization bottle were charged 80 g isooctyl acrylate (IOA), 18 g isobornyl acrylate (IBA), 2 g vinyldimethylazlactone (VDM), 100 g ethyl acetate, 0.5 g benzoyl peroxide and 0.04 g carbon tetrabromide. The bottle was purged with nitrogen, sealed and tumbled in a water bath maintained at 60° C. for 12 hours to produce a IOA/IBA/VDM terpolymer. The polymer was isolated by precipitation in isopropanol and dried under vacuum.

WORKUP

后处理

  1. customIn a glass polymerization bottle
  2. customThe bottle was purged with nitrogen
  3. customsealed
  4. customtumbled in a water bath