反応式
[B:1]12[B:4]3[B:5]4[B:2]1[C:3]234.[O-2:6].[O-2].[Ti+4:8].[CH4:9].[C-]#[Si+]>CO>[B:1]12[B:4]3[B:5]4[B:2]1[C:3]234.[O-2:6].[O-2:6].[Ti+4:8].[C:9]参加物
6
実験手順
To the boron carbide powder, 14.5 mol % of the submicron-size or nano-size titanium dioxide powder and 21.5 mol % of carbon black were incorporated, and using a methanol solvent, mixing was carried out by a planetary ball mill made of silicon carbide (SiC) at a rotational speed of 270 rpm for 1 hour, followed by drying by a evaporator and further by drying at 150° C. for 24 hours. Then, the mixture was sieved through a sieve with an opening of 250 μm to obtain a boron carbide-titanium dioxide-carbon mixed powder.
後処理
- additionmixing
- customby drying by a evaporator
- customfurther by drying at 150° C. for 24 hours
- filtrationThen, the mixture was sieved through a sieve with an opening of 250 μm
出典と根拠
- ORDレコード
- ord-527f550cf19a465ea96d73a4b1382069
- 出典データセット
- uspto-grants-2008_08
- 特許番号
- US07417002B2