反応式
[C:1]([NH2:5])(=[O:4])[CH:2]=[CH2:3].[C:6]([OH:10])(=[O:9])[CH:7]=[CH2:8]>O>[C:1]([NH2:5])(=[O:4])[CH:2]=[CH2:3].[C:6]([OH:10])(=[O:9])[CH:7]=[CH2:8]参加物
4
反応条件
- 温度
- 30 °C
実験手順
56 grams 50% acrylamide, 12 grams acrylic acid and 127 grams water were mixed, and warmed up to 30° C. Nitrogen was used to purge the flask. Then 0.7 gram ammonium persulfate in 3 grams of water and 0.7 gram sodium metabisulfite in 3 grams water were added, respectively. After 20 minutes, the reaction began to take place, the temperature slowly rose to 78° C. (max.) after stirring for 1.5 hour a 20% copolymer was thus produced with an acrylamide/acrylic acid ratio of 70/30. 7 grams NaOH in 30 grams water was then added to neutralize the copolymer.
後処理
- customto purge the flask
- additionThen 0.7 gram ammonium persulfate in 3 grams of water and 0.7 gram sodium metabisulfite in 3 grams water were added
- customslowly rose to 78° C.
出典と根拠
- ORDレコード
- ord-afb2cfbf8f8b4735958f3371f9372578
- 出典データセット
- uspto-grants-1985_05
- 特許番号
- US04515855
関連ノート
読み込み中…