Trisodium Phosphate → Tricalcium Phosphate

HRID 782

反応式

HRID 782 の反応式
[P:1]([O-:5])([O-:4])([O-:3])=[O:2].[Na+].[Na+].[Na+].[Cl-].[Ca+2:10].[Cl-]>O>[P:1]([O-:5])([O-:4])([O-:3])=[O:2].[Ca+2:10].[Ca+2:10].[Ca+2:10].[P:1]([O-:5])([O-:4])([O-:3])=[O:2]

参加物

4

実験手順

39.3 Grams of sodium phosphate were dissolved in 150 grams of water (Solution A). In a separate beaker, 22.65 grams of calcium chloride were dissolved in 150 grams of water (Solution B). Each of the above solutions were added simultaneously to 200 grams of water, while being sheared at speeds of 12,000 rpm. This shearing was necessary since the viscosity resulting from the in situ formation of tricalcium phosphate (TCP) particulates needs to be broken down into submicron size in order to be effective as a stabilizer. The amount of in situ TCP generated in this case was 16.0 grams.

出典と根拠

ORDレコード
ord-59691e7705044240a0b61a8537732528
出典データセット
uspto-grants-1998_03
特許番号
US05723252

関連ノート