反応式
[OH:1]O.[CH:3]1[CH2:10][CH2:9][CH2:8][CH2:7][CH2:6][CH2:5][CH:4]=1>C(Cl)(Cl)Cl>[CH:3]12[O:1][CH:4]1[CH2:5][CH2:6][CH2:7][CH2:8][CH2:9][CH2:10]2参加物
4
反応条件
- 温度
- 70 °C
実験手順
Crosslinked polystyrene-divinylbenzene beads substituted in the phenyl rings by arsono groups (Polymer II of Example 2 (B) above, containing 0.25 mmole As) was added to a two phase system of 1.7 g of 30% aqueous H2O2 (15 mmoles of H2O2) and cyclooctene (7.5 mmoles) in chloroform (7 ml). The mixture was heated in a closed thick-walled tube at 70° C. for 45 hours. Cyclooctene oxide (6.7 mmol, 89% yield) was obtained after 45 hours. The polymer was then filtered and reused with no apparent loss of activity (90% yield after 55 hours at 70° C.).
後処理
- additioncontaining 0.25 mmole As)
出典と根拠
- ORDレコード
- ord-4a684355f1b447ddb4c15057a804cb69
- 出典データセット
- uspto-grants-1981_08
- 特許番号
- US04286068