Ethylene carbonate → Ethylene carbonate

HRID 247714

반응식

HRID 247714 반응식
[C:1]1(=[O:6])[O:5][CH2:4][CH2:3][O:2]1>O.O.O.[O-][Sn]([O-])=O.[Na+].[Na+]>[C:1]1(=[O:6])[O:5][CH2:4][CH2:3][O:2]1.[C:1](=[O:5])=[O:2]

참가 물질

4

반응 조건

온도
175 °C

실험 절차

A 10:1 mole ratio of ethylene carbonate to polyester poly (Formrex® 11-225, a hydroxyl functional diethylene glycol adipate, MW=500, manufactured by Witco) is heated with stirring under a nitrogen atmosphere for 3.5 hours at 175° C. using 0.5 percent sodium stannate trihydrate as catalyst to give 97.3 percent ethylene carbonate conversion to a poly(alkylene carbonate) polyol with 18.7 percent carbon dioxide. The catalyst was removed as in Example 1.

후처리

  1. temperatureis heated

출처 및 근거

ORD 기록
ord-ee50f29d4fd6404fa60c2a7c438397ec
출처 데이터셋
uspto-grants-1987_11
특허 번호
US04709069

연결된 노트

불러오는 중…