반응식
[C:1]1(=[O:8])[O:7][CH2:6][CH2:5][CH2:4][CH2:3][CH2:2]1.[O:9]1[CH2:14][CH2:13][O:12][CH2:11][C:10]1=[O:15]>>[C:1]1(=[O:8])[O:7][CH2:6][CH2:5][CH2:4][CH2:3][CH2:2]1.[O:9]1[CH2:14][CH2:13][O:12][CH2:11][C:10]1=[O:15]참가 물질
3
실험 절차
The procedure in Example 5A is substantially repeated except that 45.7 grams (0.40 mole) of ε-caprolactone and 61.3 grams (0.60 mole) of p-dioxanone were used. The copolymer was dried under vacuum (0.1 mm Hg) at 80° C. for about 80 hours to remove any unreacted monomer. The copolymer had an inherent viscosity of 0.18 dL/g in HFIP at 25° C. The copolymer was a liquid at room temperature. The molar ratio of PCL/PDS was found to be 46.7/53.3 by proton NMR.
후처리
- customThe copolymer was dried under vacuum (0.1 mm Hg) at 80° C. for about 80 hours
- customto remove any unreacted monomer
- customat 25° C
- customat room temperature
출처 및 근거
- ORD 기록
- ord-3dca5811b9f14da6a82e9d0189ffa091
- 출처 데이터셋
- uspto-grants-1998_10
- 특허 번호
- US05824333
연결된 노트
불러오는 중…