Potassium Persulfate → Butyl Acrylate
Participants
| Role | Name | HCID | Charge |
|---|---|---|---|
| Reactant | Potassium Persulfate | HCID 24412 | — |
| Reactant | Butanedioic acid, 2-sulfo-, 1,4-dioctyl ester, sodium salt (1:1) | HCID 53249634 | — |
| Solvent | Water | HCID 962 | — |
| Product | Butyl Acrylate | HCID 8846 | — |
Reaction Steps
98 parts of butyl acrylate and 2 parts of tricyclodecenyl acrylate were polymerized at 65° C. for 3 hours with stirring in 154 parts of water with addition of 2 parts of sodium dioctyl sulfosuccinate (70% strength) as emulsifier and 0.5 part of potassium persulfate. This gave an approximately 40% strength dispersion. The median particle size of the latex was about 100 nm.