98 parts of butyl acrylate and 2 parts of tricyclodecenyl acrylate were polymerized at 65° C. for 3 hours with stirring in 154 parts of water with addition of 2 parts of sodium dioctyl sulfosuccinate (70% strength) as emulsifier and 0.5 part of potassium persulfate. This gave an approximately 40% strength dispersion. The median particle size of the latex was about 100 nm.

WORKUP

后处理

  1. customThis gave an approximately 40% strength dispersion