Procedure

In a polymerization vessel under nitrogen atmosphere were charged a cyclohexane solution containing 10 parts by weight of butadiene and 0.09 part by weight of n-butyllithium was added thereto. After polymerizing the mixture at 70° C. for 1 hour, a cylcohexane solution containing 90 parts by weight of styrene was added to the reaction mixture and polymerization reaction was continued at 70° C. for 2 hours. Thereafter, the polymerization reaction was stopped by adding methanol. The resulting polymer was separated from the polymer solution thus obtained by solidifying with methanol and then dried to obtain a styrene/butadiene block copolymer (weight average molecular weight: 100,000).

Workup

  1. additionwas added
  2. customAfter polymerizing the mixture at 70° C. for 1 hour
  3. additionwas added to the reaction mixture and polymerization reaction
  4. customThereafter, the polymerization reaction
  5. customThe resulting polymer was separated from the polymer solution
  6. customthus obtained
  7. customdried