HRID1348517

反应详情

EQUATION

反应方程式

HRID 1348517 的结构方程式

PROCEDURE

实验过程

In a separable flask equipped with a stirring rod, 0.080 mol (16.98 g) of DADMB, 0.010 mol (2.92 g) of APB-p and 0.010 mol (2.92 g) of APB-m were dissolved in 241 g of DMAc. With stirring 0.09 mol (19.63 g) of PMDA and 0.009 mol (2.65 g) of BPDA were added to the resulting solution to perform the polymerization, thereby obtaining a viscous, polyimide resin precursor solution (B).

WORKUP

后处理

  1. additionwere added to the resulting solution
  2. customthe polymerization