HRID325441

反应详情

EQUATION

反应方程式

HRID 325441 的结构方程式

AUXILIARIES

试剂、催化剂与溶剂

1

PROCEDURE

实验过程

The copolymer of allyl methacrylate and methacrylate was prepared by placing 5 grams of allyl methacrylate, 95 grams of methyl methacrylate, 300 milliliters of methylene chloride, and 1.0 gram of isopropyl peroxydicarbonate in a 28 ounce round bottle. The bottle was sealed. The bottle was then heated at 50 degrees Centigrade in a water bath for 18 hours. The bottle was then removed from the water bath, and the polymer isolated by extraction with methanol to precipitate polymer. The polymer was then dried under vacuum. Thereafter, the molecular weight was determined by inherent viscosity in methylene chloride versus poly(methyl methacrylate), and was found to be in excess of 500,000.

WORKUP

后处理

  1. customThe bottle was sealed
  2. temperatureThe bottle was then heated at 50 degrees Centigrade in a water bath for 18 hours
  3. customThe bottle was then removed from the water bath
  4. customthe polymer isolated by extraction with methanol
  5. customto precipitate polymer
  6. customThe polymer was then dried under vacuum