Potassium Persulfate → Butyl Acrylate
Reaction equation
C([C:9]([CH2:21][CH2:22]CCCCCC)([C:18]([O-:20])=O)C(S(O)(=O)=O)C([O-])=O)CCCCCCC.[Na+].[Na+].S(OOS([O-])(=O)=O)([O-])(=O)=O.[K+].[K+]>O>[C:18]([O:20][CH2:18][CH2:9][CH2:21][CH3:22])(=[O:20])[CH:9]=[CH2:21]Participants
4
Reactant 2
Product 1
Reagents, catalysts & solvents 1
Conditions
- Temperature
- 65 °C
Procedure
98 Parts of butyl acrylate and 2 parts of tricyclodecenyl acrylate are polymerized in 154 parts of water containing 2 parts of sodium dioctylsulfosuccinate (70% strength) as emulsifier and 0.5 part of potassium persulfate by stirring for 3 hours at 65° C. A 40% strength dispersion is obtained, the mean particle size of the latex being about 0.1 μm.
Workup
- customA 40% strength dispersion is obtained
Sources & evidence
- ORD record
- ord-a94a7621c1de40ef920f6e958629c4af
- Source dataset
- uspto-grants-1984_05
- Patent number
- US04446277
Reaction notes