HRID615482
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
CONDITIONS
反应条件
- 温度
- 200 °C
PROCEDURE
实验过程
Sodium brassylate (0.33 gram) and aluminum stearate (1.09 gram) were added to 70 grams poly(ethylene brassylate) and the mixture heated at 200° C. until a homogeneous viscous mass was obtained. The molar ratio of sodium to aluminum was 2:1. The temperature was then increased to 312° C. and the pressure reduced to 0.3-0.5 mm Hg. The depolymerization reaction was complete in about 3 hours and 88.1 percent yield ethylene brassylate was obtained.
WORKUP
后处理
- customwas obtained
- temperatureThe temperature was then increased to 312° C.
- customThe depolymerization reaction