A slurry obtained by mixing 6.2 g of a borosilicate glass powder, 56.0 g of barium titanate, 6.2 g of an acrylic organic binder containing hydroxyl groups, 3.1 g of ethanol, 3.0 g of trimethylolpropane triacrylate, 1.2 g of 2-methyl-1-[4-(methylthio)phenyl]-2-morphorinopropane-1-on, 0.3 g of 2,4-diethylthioxanthone and 0.5 g of dipropyleneglycol monomethyl ether was formed into a sheet by the doctor blade method. The sheet was dried at 100° C. to obtain a photosensitive dielectric ceramic green sheet with a thickness of 30 μm.