HRID652392
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
AUXILIARIES
试剂、催化剂与溶剂
CONDITIONS
反应条件
- 温度
- 70 °C
PROCEDURE
实验过程
13 g (0.5 mole) of vinyl acetate, 49 g (0.5 mole) of maleic acid anhydride and 0.1 g of lauroyl peroxide were dissolved in 400 cc of benzene and heated for five hours at 70° C. The copolymer was precipitated from the viscous solution with petroleum ether (80° to 100° C.). The copolymer dissolved well in diluted caustic soda.
WORKUP
后处理
- customThe copolymer was precipitated from the viscous solution with petroleum ether (80° to 100° C.)
- dissolutionThe copolymer dissolved well in diluted caustic soda