Back
HuagongsheHuagongshe Chemistry Print Report · For research reference only
HRID 894306Generated: October 25, 2026

Ethanol → Ganex E 535

https://huagongshe.com/reaction/894306

Reaction equation

Participants

RoleNameHCIDCharge
ReactantEthanolHCID 702—
ReactantN-vinyl-2-pyrrolidoneHCID 6917—
ReactantVinyl AcetateHCID 7904—
ReactantSodium HydroxideHCID 14798—
SolventDiethyl EtherHCID 3283—
ProductGanex E 535HCID 27088595%

Reaction Conditions

Temperature30 °C

Reaction Steps

Into a 2 liter round bottom flask 800 ml of ethanol, 12.8 g of sodium hydroxide pellets and 80 g of a copolymer composed of 70% N-vinylpyrrolidone and 30% vinyl acetate are introduced. The resulting reaction mixture is maintained with stirring at 30° C. for 2 hours and is then poured into 8 liters of diethyl ether to precipitate the desired polymer. After filtration the polymer is dried under reduced pressure. Yield: 95%.

Provenance & Evidence

DOI10.6084/m9.figshare.5104873.v1
Patent numberUS04283384
Source datasetuspto-grants-1981_08
ORD IDord-89a3e98d71a44dd59f10265f058e1e6b
Source noteuspto-grants-1981_08