反応式
[Al](Cl)([CH2:4][CH3:5])[CH2:2]C.[H][H].[CH3:9][CH2:10][CH2:11][CH2:12][CH2:13][CH2:14][CH3:15]>>[CH2:9]=[CH:10][CH2:11][CH2:12][CH2:13][CH2:14][CH2:4][CH3:5].[CH2:9]=[CH:10][CH2:11][CH2:12][CH2:13][CH2:14][CH:15]=[CH2:2]参加物
5
実験手順
A solution of 106.4 grams (0.95 mole) 1-octene and 5.5 grams (0.0509 mole) 1,7-octadiene (molar charge ratio 95:5) in 450 grams of heptane was polymerized with Et2AlCl (16 millimoles) and AATiCl3 (4.0 millimoles) at 50° C. for 10 hours. During the course of the reaction, hydrogen was bubbled through the reaction mixture. The conversion of the polymer was 65 percent, inherent viscosity was 2.1 dl/gram. The composition of monomers in the copolymer was 97:3 mole ratio from NMR analysis.
後処理
- customwas bubbled through the reaction mixture
出典と根拠
- ORDレコード
- ord-058afdbfbf544fed8cd88265b6b3e285
- 出典データセット
- uspto-grants-1995_06
- 特許番号
- US05428209
関連ノート
読み込み中…