反応式
[CH2:1](S)[CH2:2][CH2:3][CH2:4][CH2:5][CH2:6][CH2:7][CH2:8][CH2:9][CH2:10][CH2:11][CH3:12].CCCC[CH2:18][C:19]([C:23]([O:25]OC(C)(C)C)=[O:24])([CH2:21]C)[CH3:20]>C1(C)C=CC=CC=1>[C:23]([O:25][CH2:1][CH3:2])(=[O:24])[CH:19]=[CH2:21].[C:23]([O:25][CH2:3][CH2:4][CH2:5][CH2:6][CH2:7][CH2:8][CH2:9][CH2:10][CH2:11][CH3:12])(=[O:24])[C:19]([CH3:20])=[CH2:18]参加物
5
実験手順
350 g of toluene, 135 g of ethyl acrylate, and 15 g of n-decyl methacrylate were polymerized with stirring in a reaction flask at 50°-60° C. under argon with 0.3 g of dodecyl mercaptan as a regulator and 2 g of t-butyl perneodecanoate as initiator. After about 30 minutes of reaction, the mixture was precipitated in methanol and the polymer was dried under vacuum.
後処理
- customAfter about 30 minutes of reaction
- customthe mixture was precipitated in methanol
- customthe polymer was dried under vacuum
出典と根拠
- ORDレコード
- ord-c2b49c75adc9482d84cd3eef32fdd950
- 出典データセット
- uspto-grants-1992_08
- 特許番号
- US05141993
関連ノート