반응식
[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1.[C:9](#[N:12])[CH:10]=[CH2:11].CC(N=NC(C#N)(C)C)(C#N)C.P([O-])([O-])([O-])=O.[Ca+2].[Ca+2].[Ca+2].P([O-])([O-])([O-])=O>O>[CH2:11]=[CH:10][C:9]#[N:12].[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1참가 물질
6
실험 절차
71 parts of styrene, 29 parts of acrylonitrile, 120 parts of deionized water and 0.2 parts of azobisisobutylonitrile (AIBN) were blended. To the blend, 0.5 parts of tricalciumphosphate and 0.3 parts of mercaptan-containing chain transfer agent were added. The resultant solution was heated to 80° C. for 90 minutes and kept for 180 minutes. The resultant was washed, dehydrated and dried. Styrene-acrylonitrile copolymer (SAN) was obtained.
후처리
- additionwere added
- washThe resultant was washed
- customdried
출처 및 근거
- ORD 기록
- ord-32423f84d6c1444db24b353eaff2d0d9
- 출처 데이터셋
- uspto-grants-2006_08
- 특허 번호
- US07094818B2
연결된 노트