Azobisisobutyronitrile → Styrol-acryl-nitril

HRID 1620354
인쇄

반응식

HRID 1620354 반응식
[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1.[C:9](#[N:12])[CH:10]=[CH2:11].CC(N=NC(C#N)(C)C)(C#N)C.P([O-])([O-])([O-])=O.[Ca+2].[Ca+2].[Ca+2].P([O-])([O-])([O-])=O>O>[CH:1]([CH:11]=[CH:10][C:9]#[N:12])=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1
참가 물질실험 절차후처리출처 및 근거반응 노트

참가 물질

6

반응물 4

HCID 6547AzobisisobutyronitrileHCID 7501StyreneHCID 7855AcrylonitrileHCID 24456Tricalcium Phosphate

생성물 1

HCID 279762Styrol-acryl-nitril

시약·촉매·용매 1

HCID 962Water용매

실험 절차

76 parts by weight of styrene, 24 parts by weight of acrylonitrile, and 120 parts of deionized water are mixed. To the mixture, 0.17 parts by weight of azobisisobutylonitrile (AIBN), 0.4 parts by weight of t-dodecyl mercaptan chain transfer agent, and 0.5 parts by weight of tricalciumphosphate are added. The mixture is suspension polymerized at 75° C. for 5 hours, and a styrene-acrylonitrile (SAN) copolymer resin is obtained. The resultant copolymer is washed, dehydrated and dried to obtain SAN copolymer resin having a weight average molecular weight of 150,000 g/mol in powder form.

후처리

  1. custompolymerized at 75° C. for 5 hours

출처 및 근거

ORD 기록
ord-c580d4a94860445c8ed08c3cf458a254
출처 데이터셋
uspto-grants-2014_07
DOI
10.6084/m9.figshare.5104873.v1
특허 번호
US08772401B2

반응 노트