HRID1074627
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
CONDITIONS
反应条件
- 温度
- 314 °C
PROCEDURE
实验过程
A mixed metal catalyst comprised of aluminum stearate and lithium stearate (molar ratio 1:1) was used for the depolymerization. For the reaction aluminum stearate (1.09 g) and lithium stearate (0.36 g) were blended in 70 g poly(ethylene brassylate) at 200° C. The temperature was then raised to 314° C. while maintaining a vacuum of 0.05-0.1 mm Hg. Ethylene brassylate was obtained (40 mls during the first hour) in an 88.9% yield. Of the ethylene brassylate recovered, 90% of the product was obtained after 2 hours.
WORKUP
后处理
- temperaturewhile maintaining a vacuum of 0.05-0.1 mm Hg