Acetic Acid → 2-Propenoic acid, 2-methyl-, polymer with methyl 2-methyl-2-propenoate and methyl 2-propenoate

HRID 1938135Notes

Reaction equation

HRID 1938135 reaction equation
[C:1]([OH:4])(=[O:3])C.[CH2:5]([Si](OC)(OC)OC)[CH2:6][CH3:7].[CH2:15]([O:19][CH2:20]CC[Si](OC)(OC)OC)[CH:16]1O[CH2:17]1.N[CH2:31][CH2:32][CH2:33][Si](OC)(OC)OC.O.[I-].[Li+]>C(O)C>[C:15]([O:19][CH3:20])(=[O:3])[CH:16]=[CH2:17].[C:1]([O:4][CH3:31])(=[O:3])[C:6]([CH3:5])=[CH2:7].[C:1]([OH:4])(=[O:3])[C:32]([CH3:31])=[CH2:33]

Participants

8

Procedure

A sol-gel formulation was prepared as follows. Glacial acetic acid (108.0 grams, 1.80 mol) was added dropwise to a previously prepared, stirred mixture of propyltrimethoxysilane (489.6 grams, 2.97 mol) and 3-glycidoxypropyltrimethoxysilane (122.4 grams, 0.518 mol), followed by the dropwise addition of 3-aminopropyltrimethoxysilane (49.6 grams, 0.277 mol). The acidified silanes were then hydrolyzed by the dropwise addition of excess water (312.0 grams, 17.3 mol). The following day, the clear solution was diluted to approximately 20 wt % solids by the dropwise addition of ethanol (1046 grams) and allowed to stir in a covered vessel for 1 week. DC-190 (16 grams) was subsequently added as a plasticizer, followed by the addition of lithium iodide (9.43 grams, 0.0704 mol) to provide a "sol-gel solution".

Workup

  1. customA sol-gel formulation was prepared
  2. customa previously prepared
  3. stirringto stir in a covered vessel for 1 week
  4. additionDC-190 (16 grams) was subsequently added as a plasticizer
  5. customto provide a "sol-gel solution"

Sources & evidence

ORD record
ord-f7b61544901e485f92d15583517cd09e
Source dataset
uspto-grants-1997_12
Patent number
US05693442