反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
AUXILIARIES
试剂、催化剂与溶剂
CONDITIONS
反应条件
- 温度
- 55 °C
PROCEDURE
实验过程
Acrylic acid (105.27 g, 1.4609 moles), itaconic acid (21.12 g, 0.1623 mole), Wako V-50 (0.4403 g, 1.623 millimole), and 812 ml of water, which has been acidified to pH 2.0 with hydrochloric acid, are added to a 2 liter three-necked round-bottomed flask. The necks are fitted with a thermometer, a stopper, and a gas inlet/outlet adapter capable of bubbling gas through a liquid in the flask and venting it. The solution is deaerated by passage of nitrogen gas and is then placed under an atmosphere of argon. The solution is heated to 55° C. and maintained at this temperature for 15 hours. The viscous solution of copolymer is cooled to ambient temperature and is freeze dried to give 121.57 g of poly(acrylic acid-itaconic acid) copolymer as a colorless solid. The mass average molecular weight, as determined by low angle laser light scattering on a dialyzed portion in 0.2 Molar sodium chloride in water (refractive index=1.3344, dn /dc =0.1683), is 821,600.
WORKUP
后处理
- additionare added to a 2 liter three-necked round-bottomed flask
- customThe necks are fitted with a thermometer
- customa stopper, and a gas inlet/outlet adapter capable of bubbling gas through a liquid in the flask
- temperaturemaintained at this temperature for 15 hours
- temperatureThe viscous solution of copolymer is cooled to ambient temperature
- customdried