HRID254137
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
AUXILIARIES
试剂、催化剂与溶剂
PROCEDURE
实验过程
19 g of sodium styrenesulfonate (SSNa) (available from Sigma-Aldrich Corp.) and 1 g of branched perfluorooctene (heptafluoro-3,3-bis(trifluoromethyl)-1-hexene) are fully dissolved in 0.24 L of dimethylsulfoxide (DMSO) with heating. Then, 0.1 g of azobisisobutyronitrile (AIBN) is added dropwise to the DMSO solution. The monomers are polymerized for 24 hours or more. The polymerization is carried out varying the content of the branched perfluorooctene (5, 10, and 20 wt %).
WORKUP
后处理
- temperaturewith heating
- customThe monomers are polymerized for 24 hours or more