375 °C

PROCEDURE

实验过程

An iron containing ZSM-5 catalyst was prepared by the following method: about 10 g of the same HZSM-5 as that of Example 1 was heated in a stream of dry air to 375° C. for 4 hours and then was cooled to room temperature. A solution of 0.1667 g of ferrocene (dicyclopentadienyliron) in 30 g dry toluene was then added to the dried zeolite and the slurry was mixed at room temperature overnight. Excess toluene was allowed to evaporate at room temperature to give a toluene/ferrocene wetted zeolite. The recovered solid was then calcined in a stream of dry air at about 538° C. for about 6 hours to produce the desired iron containing catalyst, Catalyst B. The iron loading of this catalyst is about 0.45 wt. %.

WORKUP

后处理

  1. temperaturewas cooled to room temperature
  2. additionthe slurry was mixed at room temperature overnight
  3. customto evaporate at room temperature