反応式
[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1.[C:9](#[N:12])[CH:10]=[CH2:11].CC(N=NC(C#N)(C)C)(C#N)C.P([O-])([O-])([O-])=O.[Ca+2].[Ca+2].[Ca+2].P([O-])([O-])([O-])=O>O>[CH2:11]=[CH:10][C:9]#[N:12].[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1参加物
6
実験手順
71 parts of styrene, 29 parts of acrylonitrile, 120 parts of deionized water and 0.2 parts of azobisisobutylonitrile (AIBN) were blended. To the blend, 0.5 parts of tricalciumphosphate and 0.3 parts of mercaptan-containing chain transfer agent were added. The resultant solution was heated to 80° C. for 90 minutes and kept for 180 minutes. The resultant was washed, dehydrated and dried. Styrene-acrylonitrile copolymer (SAN) was obtained.
後処理
- additionwere added
- washThe resultant was washed
- customdried
出典と根拠
- ORDレコード
- ord-32423f84d6c1444db24b353eaff2d0d9
- 出典データセット
- uspto-grants-2006_08
- 特許番号
- US07094818B2
関連ノート