反応条件

温度
150 °C

実験手順

Glycolide (0.21 moles) was mixed with ε-caprolactone (4.0 moles) and a catalytic amount of stannous octoate (0.8 mole) and glycolic acid (0.40 moles). The system was heated to 150° C. and was stirred at this temperature for 14 hours. At the conclusion of the reaction, the unreacted monomer was removed by heating at 120° C. under reduced pressure for 1 hour. The resulting polymer had a peak melting temperature of 54.3° C. as measured by DSC.

後処理

  1. customAt the conclusion of the reaction
  2. customthe unreacted monomer was removed
  3. temperatureby heating at 120° C. under reduced pressure for 1 hour

出典と根拠

ORDレコード
ord-515a6a6c9ec040f88ec84ca01eb6da11
出典データセット
uspto-grants-2001_10
特許番号
US06299631B1

関連ノート

読み込み中…