HRID1610781

反应详情

EQUATION

反应方程式

HRID 1610781 的结构方程式

AUXILIARIES

试剂、催化剂与溶剂

1

CONDITIONS

反应条件

温度
67 °C

PROCEDURE

实验过程

9 g of acrylic acid, 1 g of methyl acrylate, 50 g of isobutyl methyl ketone, 50 g of propylene glycol methyl ether acetate and 3.0 g of AIBN were combined and heated to about 67° C. for 3 hours under an inert atmosphere (e.g., nitrogen gas). The precipitated polymer was washed with ethyl ether and vacuum dried to obtain pure poly(acrylic acid/methyl acrylate) resin (weight average molecular weight: 7200, yield: 54%).

WORKUP

后处理

  1. washThe precipitated polymer was washed with ethyl ether and vacuum
  2. customdried