HRID2254020
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
AUXILIARIES
试剂、催化剂与溶剂
PROCEDURE
实验过程
this polymer material was produced by adding to 320 g xylene at 100° C. the monomer solution and a catalyst solution over a period of 3 hours. The monomer solution contained 2.900 g ethyl acrylate, 76 g acrylonitrile, 76 g acrylic acid and 3 g laurylmercaptan. The catalyst solution contained 26 g laurylperoxide and 7 g butylperbenzoate in 273 g of xylene. The material was highly viscous with comonomer proportions of 95:2.5:2.5.