HRID491251

反应详情

EQUATION

反应方程式

HRID 491251 的结构方程式

CONDITIONS

反应条件

温度
67 °C

PROCEDURE

实验过程

3 g of 4-bromostyrene, 4 g of acrolein, 3 g of methacrylate and 0.2 g of AIBN were sufficiently mixed with 50 g of PGMEA. The mixture was polymerized by heating the mixture at 67° C. for 8 hours. After completion of the polymerization, the polymerization product was precipitated in n-hexane, filtered, and dried in vacuo to give a poly(bromostyrene-acrolein-methacrylate) copolymer.

WORKUP

后处理

  1. customThe mixture was polymerized
  2. customAfter completion of the polymerization
  3. customthe polymerization product was precipitated in n-hexane
  4. filtrationfiltered
  5. customdried in vacuo